The process of the surface oxidizing of Nd thin films used in X-ray laser experiment is studied through AES method combined with Ar ion beam etching. The experimental results, which agree well with that of RBS, show that the surface oxidisation of Nd is saturated just 20~30 minutes after the sample exposed in air, the max thickness of oxide layer is about 20nm, and the main composition of oxide layer is NdO.